Sandvik-By mechanical properties
|
Mechanical strength |
|||
Proof strength |
Tensile |
Elongation |
|
Designation |
Rp0.2 |
Strength, Rm |
A |
Sandvik |
MPa, min. |
MPa |
%.min |
Austenitic stainless steels (prefix standard THT,TST,TST-E or THE) |
|||
3R12 |
210 |
515-680 |
45 |
3R60 |
220 |
515-690 |
45 |
3R65 |
220 |
515-690 |
45 |
6R35 |
210 |
515-690 |
45 |
5R75 |
220 |
510-710 |
45 |
5R10 |
210 |
515-690 |
45 |
3R19 |
275 |
550-750 |
40 |
5R60 |
220 |
515-690 |
40 |
3R64 |
220 |
515-690 |
35 |
3R68 |
285 |
580-800 |
35 |
8R40 |
220 |
515-690 |
35 |
8R41 |
210 |
510-690 |
35 |
3R60 U.G. |
190 |
490-690 |
40 |
Duplex stainless steels (prefix standard THT,TST,TST-E or THE) |
|||
SAF 2304 |
400 |
600-820 |
25 |
SAF 2205 |
450 |
680-880 |
25 |
SAF 2507 |
550 |
800-1000 |
25 |
3RE60 |
450 |
700-800 |
30 |
High-alloy austenitic stainless steels and nickel alloys (prefix standard THT, TST, TST-E or THE) |
|||
2RK65 |
230 |
520-720 |
35 |
Sanicro 28 |
220 |
550-750 |
40 |
2RE10 |
210 |
500-670 |
35 |
2RE69 |
270 |
580-780 |
30 |
254 SMO |
310 |
655-850 |
35 |
Sanicro 30 |
205 |
520-690 |
30 |
Sanicro 41 |
240 |
590-750 |
30 |
Sanicro 69 |
240 |
>585 |
30 |
High temperature grades (prefix standard THR) |
|||
4C54 |
275 |
500-700 |
20 |
7RE10 |
220 |
515-750 |
35 |
253 MA |
310 |
650-850 |
40 |
353 MA |
270 |
650-750 |
40 |
Sanicro 31HT |
170 |
500-700 |
35 |
8RE18 |
205 |
>515 |
35 |
Esshete 1250 |
220 |
540-740 |
35 |
Sanicro 70 |
245 |
>560 |
35 |
Special grades for machining (prefix standard THB) |
|||
210 |
515-680 |
40 4) |
|
220 |
515-690 |
40 4) |
|
220 |
515-690 |
40 4) |
|
220 |
510-710 |
35 |
|
450 |
680-880 |
25 |
|
10RE51 |
485 |
620-800 |
20 |
Sandvik -> Standard,Mechanical Properties